TL;DR: Standard 316L (UNS S31603) is not an implant material. 316LVM (UNS S31673) is the implant-grade version, specified by ASTM F138 for bar and wire and by ISO 5832-1. It is a different chemistry, with higher chromium, nickel and molybdenum and tighter limits on phosphorus and sulphur. It must also meet a composition-based pitting criterion, Cr + 3.3 × Mo ≥ 26, and contain no delta ferrite, chi or sigma phase. A 316L heat cannot meet that criterion, and even an F138 heat at the bottom of its ranges fails it, so the certificate must show the calculation. The steel is remelted, by vacuum or electroslag remelting (ESR), to reach the cleanliness implants need. Order by UNS S31673 to ASTM F138 or ISO 5832-1, never as “316L surgical steel”.
316LVM vs 316L is not a question of premium versus standard 316L. The two are different materials that share a family name.
316L is the low-carbon version of Type 316. It is used for process equipment, pharmaceutical plant and surgical instruments.
316LVM is a separately specified alloy, UNS S31673. Its chemistry is rebalanced and tightened for implantation, and it is melted and tested to prove cleanliness and phase purity that 316L is never required to show.
This guide explains what ASTM F138 and ISO 5832-1 require that 316L does not. It covers why the composition-based pitting criterion is the check most certificates skip, and what remelting adds. It also shows where stainless steel stops and titanium or cobalt alloys take over, and what an implant manufacturer should see on the purchase order and certificate.
Is 316L Stainless Steel Implant Grade?
No. Standard 316L (UNS S31603) is not implant grade; implant-grade stainless steel is UNS S31673, commonly called 316LVM, supplied to ASTM F138 or ISO 5832-1.
ASTM F138-19 is titled Standard Specification for Wrought 18Chromium-14Nickel-2.5Molybdenum Stainless Steel Bar and Wire for Surgical Implants (UNS S31673). It covers the chemical, mechanical and metallurgical requirements for bar and wire used to manufacture surgical implants.
ISO 5832-1:2024 is the international counterpart, Implants for surgery: Metallic materials, Part 1: Wrought stainless steel. ISO states that the alloy it describes corresponds to UNS S31673 in ASTM F138 and ASTM F139.
316L has its own place in medicine. Stainless France lists 316L, grade 1.4404, against ASTM F899, the specification for stainless steels used in surgical instruments. It names the medical industry’s instrumentation as its application, not implantation.
The practical line is simple:
-
instruments that leave the body can be 316L
-
implants that stay in the body are UNS S31673
“Surgical steel” is not a specification. The search term is heavily used for jewellery and piercing products, and a label of “316L surgical steel” says nothing about whether the material meets F138.
316L vs 316LVM Comparison Table
316LVM carries more chromium, nickel and molybdenum than 316L, and much tighter limits on phosphorus and sulphur.
| Element, % | 316L, EN 1.4404 (Stainless France) | 316LVM, UNS S31673 to ASTM F138 / ISO 5832-1 (Stainless France) |
|---|---|---|
| Carbon | max 0.03 | max 0.03 |
| Chromium | 16.5 to 18.0 | 17.0 to 19.0 |
| Nickel | 10.5 to 13.0 | 13.0 to 15.0 |
| Molybdenum | 2.0 to 2.5 | 2.25 to 3.0 |
| Manganese | max 2.0 | max 2.0 |
| Silicon | max 1.0 | max 0.75 |
| Phosphorus | max 0.045 | max 0.025 |
| Sulphur | max 0.015 | max 0.010 |
| Nitrogen | max 0.11 | max 0.10 |
| Copper | not specified | max 0.50 |
| Pitting criterion | none | Cr + 3.3 × Mo ≥ 26 |
| Phase requirement | none | no delta ferrite, chi or sigma phase (ASTM F138) |
| Typical melt route | EAF followed by AOD (Stainless France) | Remelted, by ESR or vacuum remelting |
| Medical use | Instruments (ASTM F899) | Implants (ASTM F138, ISO 5832-1) |
The American 316L specifications allow an even wider window than the EN grade: 16.0 to 18.0% chromium, 10.0 to 14.0% nickel and 2.0 to 3.0% molybdenum. That makes the gap to F138 larger still.
The designations also differ. 316L is UNS S31603 and EN 1.4404. 316LVM is UNS S31673, and the European equivalent is 1.4441, X2CrNiMo18-15-3.
What ASTM F138 and ISO 5832-1 Require That 316L Does Not
ASTM F138 adds three layers that 316L specifications do not carry: an implant-specific chemistry with a pitting criterion, a phase-purity requirement, and mechanical and metallurgical testing tied to implant manufacture.
-
Chemistry balanced for passivity. Chromium, nickel and molybdenum are raised and residual phosphorus and sulphur cut. The alloy then stays fully austenitic and resists pitting in body fluid. Stainless France lists the F138 / ISO 5832-1 requirement that Cr + 3.3 × Mo must be at least 26.
-
No delta ferrite, chi or sigma. ASTM F138 requires the material to contain no delta ferrite, chi or sigma phases when examined by metallography. 316L specifications carry no such requirement.
-
Mechanical properties by condition. F138 bar and wire are furnished hot-worked, annealed, cold-worked or extra hard. The specification requires ultimate tensile strength, yield strength, elongation and Brinell hardness to be determined. The ASTM record for F138-19 also lists AMS 2630 and AMS 2632, the aerospace ultrasonic inspection standards, among its referenced documents.
-
Finish. F138 allows bar and wire to be supplied cold-drawn, pickled, ground, or ground and polished.
The difference between 316L and 316LVM is not a certificate label. It is a set of tests the heat has to pass.
The Cr + 3.3Mo ≥ 26 Rule: The Check Most Certificates Skip
The composition-based pitting criterion is the single most useful check on an implant-grade stainless steel certificate. Even a heat inside every F138 element range can fail it.
Take a standard 316L heat at mid-range EN 1.4404 chemistry, 17.2% chromium and 2.2% molybdenum:
-
17.2 + (3.3 × 2.2) = 17.2 + 7.26 = 24.5
-
316L cannot reach 26 even at its maximums of 18.0% chromium and 2.5% molybdenum: 18.0 + 8.25 = 26.25, just clear, but only if every limit is pushed to the top at once.
Now take a heat inside the F138 ranges but near their minimums, 17.2% chromium and 2.4% molybdenum:
-
17.2 + (3.3 × 2.4) = 17.2 + 7.92 = 25.1, which fails.
A heat at 17.6% chromium and 2.6% molybdenum passes: 17.6 + 8.58 = 26.2.
The consequence for buyers is direct. An F138 certificate must show the actual chromium and molybdenum and the calculated value, not simply “conforms”. A melter producing implant bar has to aim both elements toward the upper half of their ranges. That is one reason implant-grade heats are melted as dedicated heats rather than selected from ordinary 316L production.
Why Remelting Matters: Cleanliness, Homogeneity and Fatigue
Implant-grade 316LVM is remelted after primary melting to reduce inclusions and segregation, because inclusions act as initiation sites for fatigue cracks and pits in a cyclically loaded implant.
The “VM” in 316LVM historically referred to vacuum melting, and some producers still supply vacuum-remelted material. Alleima describes its 316LVM as vacuum remelted, with bar and wire supplied to ASTM F138.
Remelting by electroslag is equally established. Stainless France states that its 1.4441 grade is remelted by an ESR-type consumable electrode. It says this increases cleanliness and homogeneity, which are essential for fatigue strength, biocompatibility and corrosion resistance. It supplies the grade with a fine, homogeneous grain size of at least ASTM index 5.
For the buyer, the melt route label matters less than the evidence. The evidence that should appear on a certificate is:
-
the remelting process used
-
the inclusion rating and its test method
-
the grain size
-
the metallographic confirmation of no delta ferrite, chi or sigma
Supreme Engineering’s position is that material for orthopedic implants must be remelted through ESR. For how electroslag remelting removes inclusions and why aerospace and medical specifications demand remelted material, see Why ESR and VIM Remelting Matter for Aerospace, Defence and Medical Special Steel.
Where 316LVM Stops: Titanium, Cobalt-Chrome and MP35N
316LVM is the cost-effective implant alloy for temporary fixation and many trauma devices, but load-bearing, long-term and high-fatigue implants move to titanium, cobalt-chromium or MP35N.
| Material | Specification | Typical role |
|---|---|---|
| 316LVM stainless steel | ASTM F138, ISO 5832-1 | Bone screws, plates, pins, nails, wires and fixation devices |
| Titanium-6Al-4V ELI (UNS R56401) | ASTM F136 | Long-term implants where lower modulus, lower density and nickel-free chemistry matter |
| Wrought cobalt-chromium-molybdenum | ASTM F1537 | Articulating and high-wear components |
| MP35N (UNS R30035) | ASTM F562, ISO 5832-6 | Very high strength wire and small components, such as leads and cables |
ASTM F136 covers wrought annealed titanium-6aluminium-4vanadium ELI (extra low interstitial) alloy for surgical implants. It is supplied as strip, sheet, plate, bar, forging bar and wire.
MP35N is a registered trademark of SPS Technologies. It is a nickel-cobalt-chromium-molybdenum alloy used where 316LVM and titanium lack the strength. For how MP35N’s supply condition governs its properties, see MP35N to AMS 5845 vs NACE MR0175. Supreme Engineering supplies MP35N round bar.
What an Implant OEM Needs on the Certificate
An implant manufacturer’s regulatory file needs a material certificate that proves the heat meets ASTM F138 or ISO 5832-1 in full, traceable to the melt, not a 316L certificate with a medical label. The certificate should show:
-
UNS S31673 and the specification with edition. For example ASTM F138-19 or ISO 5832-1:2024. ISO 5832-1:2024 is the sixth edition, published April 2024, with a corrected version in June 2025.
-
Heat number and melting mill, including the remelt route and the name of the producer of the final remelt.
-
Actual chemistry for every limited element. This includes phosphorus, sulphur, nitrogen and copper, plus the calculated Cr + 3.3 × Mo value against the minimum of 26.
-
Metallography. Confirmation of no delta ferrite, chi or sigma phase, and the grain size.
-
Inclusion rating. The method and results.
-
Mechanical properties in the delivered condition, annealed, cold-worked or extra hard. These are tensile, yield, elongation and hardness.
-
Ultrasonic testing to the standard and class required, with the result.
-
Certificate type. EN 10204 3.1 at minimum, validated by an inspection representative independent of production.
316LVM Bar Purchase Order Checklist
A correct implant-grade order names the alloy by UNS number, cites the implant specification, states the condition and finish, and makes the pitting criterion and phase check explicit acceptance items.
-
Grade. “UNS S31673 (316LVM / 1.4441)”. Do not write “316L” or “surgical steel”.
-
Specification. ASTM F138 (bar and wire) or ISO 5832-1, with the edition your technical file references.
-
Condition and finish. Annealed, cold-worked or extra hard; cold-drawn, ground, or ground and polished.
-
Size and tolerance. Diameter, tolerance, straightness and length.
-
Chemistry acceptance. Actual values for all limited elements and the calculated Cr + 3.3 × Mo ≥ 26 on the certificate.
-
Microstructure acceptance. No delta ferrite, chi or sigma phase, and grain size reported.
-
Cleanliness. Remelt route stated, with the inclusion rating method and results.
-
Non-destructive testing. Ultrasonic testing standard and acceptance class. Supreme Engineering ultrasonically tests 100% of bars with back-wall echo, DGS and flat-bottom-hole methods, per its testing facilities page.
-
Traceability. EN 10204 3.1 certificate naming the melting mill and heat. For how to check that a certificate comes from the mill that melted the bar, see who actually manufactures special steel and superalloy round bar in India.
Supreme Engineering lists 316LVM, 316LRM and 316L stainless steel bar.
Frequently asked questions
- Is 316L stainless steel implant grade?
- No. Standard 316L, UNS S31603 and EN 1.4404, is a general-purpose low-carbon stainless steel used for process equipment and for surgical instruments under ASTM F899. It is not specified for implantation.
Implant-grade stainless steel is UNS S31673, commonly called 316LVM, supplied to ASTM F138 for bar and wire or to ISO 5832-1. Compared with 316L, it has:
higher chromium (17.0 to 19.0%), nickel (13.0 to 15.0%) and molybdenum (2.25 to 3.0%)
tighter phosphorus and sulphur limits
a pitting criterion of Cr + 3.3 × Mo ≥ 26
no delta ferrite, chi or sigma phase
A product sold as “316L surgical steel” does not meet those requirements unless certified to F138 or ISO 5832-1. - What is the difference between 316L and 316LVM?
- 316LVM is a different alloy from 316L, not a cleaner version of it. Its UNS number is S31673 against S31603 for 316L, and its European number is 1.4441 against 1.4404.
The chemistry is rebalanced. 316LVM carries 17.0 to 19.0% chromium, 13.0 to 15.0% nickel and 2.25 to 3.0% molybdenum, with phosphorus held to 0.025% and sulphur to 0.010%. It must satisfy Cr + 3.3 × Mo ≥ 26 and contain no delta ferrite, chi or sigma phase.
It is also remelted, by vacuum or electroslag remelting, to reduce inclusions. 316L is typically melted in an electric arc furnace and refined by AOD, with none of these implant requirements. - What does ASTM F138 cover?
- ASTM F138-19 covers the chemical, mechanical and metallurgical requirements for wrought 18 chromium, 14 nickel, 2.5 molybdenum stainless steel bar and wire (UNS S31673) used to manufacture surgical implants. Bar and wire are furnished hot-worked, annealed, cold-worked or extra hard, with cold-drawn, pickled, ground, or ground and polished finishes.
The heat analysis must meet the specified composition. The material must contain no delta ferrite, chi or sigma phase when examined by metallography. Tensile strength, yield strength, elongation and Brinell hardness must be determined.
The companion specification ASTM F139 covers sheet and strip. ISO 5832-1 covers the same alloy internationally. - What does “VM” stand for in 316LVM?
- “VM” stands for vacuum melted, from the original production route for implant-grade 316L-type steel. Today it is a trade designation, not a melt requirement you can rely on from the name alone.
Some producers supply vacuum-remelted material, as Alleima does for its 316LVM. Others remelt by electroslag: Stainless France states that its 1.4441 grade is ESR-remelted to increase cleanliness and homogeneity.
The specification that governs the material is ASTM F138 or ISO 5832-1, and the alloy is UNS S31673. Check the certificate for the actual remelt route, inclusion rating and phase check rather than inferring them from the letters “VM”. - Is ISO 5832-1 the same as ASTM F138?
- They describe the same alloy. ISO states that the wrought stainless steel in ISO 5832-1 corresponds to UNS S31673 in ASTM F138 and ASTM F139, and to material number 1.4441.
They are separate documents with their own editions and test methods. ISO 5832-1:2024 is the sixth edition, published April 2024, with a corrected version in June 2025. ASTM F138-19 is the active ASTM edition.
Implant manufacturers should order to whichever specification their regulatory file and design history reference, and state the edition. Where both apply, the certificate should confirm compliance with both. - When should an implant use titanium or cobalt-chrome instead of 316LVM?
- 316LVM is widely used for bone screws, plates, pins, nails, wires and temporary fixation devices, where its cost, formability and strength are an advantage.
Designers move to other alloys for long-term, load-bearing and high-fatigue implants:
Titanium-6Al-4V ELI (ASTM F136): lower density and modulus, and it is nickel-free.
Wrought cobalt-chromium-molybdenum (ASTM F1537): superior wear resistance for articulating components.
MP35N (ASTM F562, ISO 5832-6): very high strength in small sections such as wire and cable.
The choice is a design and regulatory decision for the implant manufacturer, based on load, duration, patient factors and the device’s clinical history.